Core Material / Technical Data
Data Sheet Cu (Copper, pure and alloyed) 1)
| Electrolytic Tough Pitch Copper | Oxygen-free Copper | Oxygen-free Copper select. *) |
Copper with Ag *) | OF-Copper with Mg |
||
| Standard Specifications | DIN / EN | Cu-ETP1 | Cu-OF1 | Cu-OF1 select. |
CuAg0,1 | CuMg0,4 |
| CW003A | CW007A | - | CW013A | CW128C | ||
| UNS | C11040 | C10100 | - | C11600 | C18661 | |
| Nominal Composition | [%] | ≥99,90 Cu | ≥99,95 Cu | ≥99,95 Cu | 0,1 Ag balance Cu |
0,55 Mg balance Cu |
| Electrical Conductivity 2) | 58 | 58 | 58 | 57 | 37 | |
| Spec. electrical Conductivity 2) | [% IACS] | 100 | 100 | 100 | 98 | 64 |
| Thermal Conductivity | [W/m K] | 390 | 390 | 390 | 390 | 380 |
| Coefficient of thermal Expansion 3) | [10-6 / K] | 17 | 17 | 17 | 17 | 18 |
| Tensile Strength annealed |
[N/mm2] | 240 | 240 | 240 | 240 | 310 |
| Elongation annealed |
[%] | 30 | 30 | 30 | 30 | 30 |
| Tensile Strength hard |
[N/mm2] | 450 | 450 | 450 | 450 | 560 |
| Density | [g/cm3] | 8,89 | 8,89 | 8,89 | 8,89 | 8,89 |
1) Wire diameter tested: 0,8 mm.
2) At 20 °C.
3) Temperature range 20 °C - 200 °C.
*) Higher temperature resistivity.