Data Sheet Cu (Copper, pure and alloyed)
| |
|
Electrolytic Tough Pitch Copper |
Oxygen-free Copper |
Oxygen-free Copper select. *) |
Copper with Ag *) |
OF-Copper with Mg |
| Standard Specifications |
DIN / EN |
Cu-ETP1 |
Cu-OF1 |
Cu-OF1 select. |
CuAg0,1 |
CuMg0,4 |
| CW003A |
CW007A |
- |
CW013A |
CW128C |
| UNS |
C11040 |
C10100 |
- |
C11600 |
C18661 |
| Nominal Composition |
[%] |
≥99,90 Cu |
≥99,95 Cu |
≥99,95 Cu |
0,1 Ag balance Cu |
0,55 Mg balance Cu |
| Electrical Conductivity 2) |
[m/(Ohm mm2)] |
58 |
58 |
58 |
57 |
37 |
| Spec. electrical Conductivity 2) |
[% IACS] |
100 |
100 |
100 |
98 |
64 |
| Thermal Conductivity |
[W/m K] |
390 |
390 |
390 |
390 |
380 |
| Coefficient of thermal Expansion 3) |
[10-6 / K] |
17 |
17 |
17 |
17 |
18 |
Tensile Strength annealed |
[N/mm2] |
240 |
240 |
240 |
240 |
310 |
Elongation annealed |
[%] |
30 |
30 |
30 |
30 |
30 |
Tensile Strength hard |
[N/mm2] |
450 |
450 |
450 |
450 |
560 |
| Density |
[g/cm3] |
8,89 |
8,89 |
8,89 |
8,89 |
8,89 |
1) Wire diameter tested: 0,8 mm.
2) At 20 °C.
3) Temperature range 20 °C - 200 °C.
*) Higher temperature resistivity.